Laser Welding Prong Repairs Project | |
| Use a separating disk to grind the prong flat. Place a redi-prong on a metal surface and tap gently to remove any flashing on bottom. Lay the redi-prong on the prong and check for tight fit. |
| To tack redi-prong in place hold it with fine tweezers and shoot with a laser at the joint between the bottom of the redi-prong and the old prong. |
| Side view ofprong tacked in place. Check to make sure the prong is tight against stone and tighten if necessary. |
| Turn the ring around and shoot the laser down from the top to finish the seam between the new prong tip and the old prong. |
| Place 30ga wire on welded joint and fill several passes with laser shooting from the side, until you achieve the original contour of the prong. |
| No pumice wheel should be needed to finish the back of the prong. I used a 6-inch knife edge wheel to concentrate the polishing on the prong only and then put it right into the cleaner. |
| Finished product for new prongs took less then ten minutes from start to finish. |
You assume all responsibility and risk for the use of the safety resources available on or through this web page. The International Gem Society LLC does not assume any liability for the materials, information and opinions provided on, or available through, this web page. No advice or information provided by this website shall create any warranty. Reliance on such advice, information or the content of this web page is solely at your own risk, including without limitation any safety guidelines, resources or precautions, or any other information related to safety that may be available on or through this web page. The International Gem Society LLC disclaims any liability for injury, death or damages resulting from the use thereof.