Alloying Gold for Granulation


An alloy is by definition a mixture of two or more metals to create different strengths and colors. For granulation, the following formula is preferred. It is important to start with pure metals. Even trace amounts of impurities can result in flaws in the metal.

7 Minute Read

HomeLearning CenterAlloying Gold for Granulation
By Ronda CoryellMore from this author
Updated on

An alloy is by definition a mixture of two or more metals to create different strengths and colors. For granulation, the following formula is preferred. It is important to start with pure metals. Even trace amounts of impurities can result in flaws in the metal.

Preparing & Measuring Alloys

For granulation, the following formula is preferred:
  • Pure Copper 0.5 dwt ( Fig. 1)
  • Fine Silver 1.5 dwt ( Fig. 2)
  • 24kt Gold 22 dwt (Fig. 3)

The quantity of 22kt produced is 24 dtw total weight. If using a tray to weigh, be sure to reset the scale to zero with the tray before adding the metal.

Alloying 22KT Gold for GranulationFig. 1
0.5 dwt Pure Copper
Alloying 22KT Gold for GranulationFig. 2
1.5 dwt Fine Silver
Alloying 22KT Gold for GranulationFig. 3
22 dwt 24kt Pure Gold.
Alloying 22KT Gold for GranulationFig. 4
Copper w/mix of boric acid and alcohol
The copper must be prepared prior to using. A mixture of boric acid and alcohol (1 tsp boric acid to 1 oz denatured alcohol is a good consistancy) is used to coat the copper and ignite. Just enough mixture to paint the surface of the copper is necessary. (Fig. 4)

This leaves a protective layer the guards against oxidation. If the copper is allowed to oxidize before it is melted, it can create copper spots in the cast ingot. The copper is now ready to use. The copper is NOT added to the alloy mixture until the gold-silver alloy mixture is MOLTEN.

Making a Charcoal Ignot Mold

Alloying 22KT Gold for GranulationFig. 5
Carving the sheet ingot
To make an ingot mold, use a compressed charcoal block. It is much harder than a standard charcoal block. It is much harder and will hold up better under high heat when making sheet ingots. Use a sharp 1 ½" chisel, scrape the charcoal down in thin, even layers. (Fig. 5) The bottom should be flat and smooth. Make the area approximately 1/8″ deep and 2″ long. A thin, wide, flat ingot is preferred. A thick ingot is harder to work down to make sheet.
Alloying 22KT Gold for GranulationFig. 6
Carving the wire ingot
Various sized wire molds can be carved into the same charcoal block. Using the tip of a screwdriver in the same manner that the chisel is used for the sheet ingot mold, scrape out a depression ¼" deep and 2 ½" long. (Fig. 6)

It should be as deep as it is wide in order to pour an even wire ingot.

Mixing The Alloys

Alloying 22KT Gold for GranulationFig. 7
Preheating the mold
Always preheat the charcoal block to a glowing red efore adding metal. (Fig 7)

This helps reduce the length of time that the metal will be exposed to the torch, thus reducing the degree of oxidation.

Alloying 22KT Gold for GranulationFig. 8
Adding the 24kt Gold to the molten Fine Silver
Melt the fine silver first. Then the gold can be fed into the alloy mixture a little at a time. (Fig. 8) The gold-fine silver alloy does not oxidize.

Once the precious metals are well mixed, add the prepared copper. It is quickly absorbed into the alloy mixture.

Alloying 22KT Gold for GranulationFig. 9
Mixing copper into alloy
Mix thoroughly with a carbon, graphite, or quartz rod or a wooden stick as you add the copper. (Fig. 9) I prefer wooden chopsticks kept soaking nearby in a glass of water.

The flame uses the oxygen present, preventing oxides from forming.

Alloying 22KT Gold for GranulationFig. 10
Skimming impurities off to side
Once the molten metal is well mixed, skim the surface with the wooden stir stick to move impurities to the side. (Fig. 10)

 

Alloying 22KT Gold for GranulationFig. 11
Placing another charcoal block on top
Keep the flame on the metal as you cover it with another piece of charcoal block large enough to cover the area surrounding the ingot. (Fig. 11) It does not have to be compressed charcoal, but it should have a flat, smooth surface.

Press down on the pool of molten metal to spread the metal flat while creating a purifying reduction atmosphere where little or no oxygen can get to the surface of your metal. This reduces the amount of oxidation on the surface of your ingot.

Making Wire Ingot

Alloying 22KT Gold for GranulationFig. 12
Scrap metal being formed into wire ingot
Unless using scrap, it is impossible to mix the alloy in a wire mold, therefore it should be poured using a hand-held crucible.

Scrap 22kt sheet and wire can easily be re-melted in a wire ingot. (Fig. 12)

Alloying 22KT Gold for GranulationFig. 13
Melting the metal until it balls up
Work the flame from end to end until the metal "balls up".

(Fig. 13) When the metal "balls up", place another charcoal block on top of it to flatten the metal into the mold and prevent oxidation.

Alloying 22KT Gold for GranulationFig. 14
Placing another charcoal block on top
Keep the flame on top of the metal until the other charcoal block is on top because as soon as the flame is taken away, the metal solidifies. (Fig. 14)

 

Alloying 22KT Gold for GranulationFig. 15
Ingot ready to quench
The finished wire ingot is now ready to quench, forge, roll, and draw down to the desired size. (Fig.15) Quench the ingot in water as soon as it is no longer glowing red.

This retains the crystallized structure of the metal. If the ingot is quenched too rapidly, stress cracks can form.

Making Larger Quantities

Alloying 22KT Gold for GranulationFig. 16
Depositing soot on wire ingot mold
Steel molds must be prepared by oiling, using silicone spray, or depositing a layer of soot on the interior of the mold surface, graphite molds need no preparation.

The steel molds should be preheated in order to get a good pour. To deposit a layer of soot, simply cover the air intake valve on your torch to create soot. (Fig. 16)

Alloying 22KT Gold for GranulationFig. 17
Pouring from a hand held crucible
A hand-held crucible must be preheated before adding metals. Pour the molten metal in a smooth, even motion, keeping the flame on the metal throughout the entire pour; concentrate the flame on the point of the spout of the crucible.

(Fig. 17) The spout of the crucible should be poured as close as possible to the mold to prevent premature cooling of the metal and to reduce the chance of spillage. Always have the mold in a tray to catch any spills. If the tray is filled with a layer of sand, the gold will be easy to retrieve.

Alloying 22KT Gold for GranulationFig. 18
Using an electromelt furnace
An electromelt furnace can make it possible to pour multiple ounces of both sheet and wire with the same melt. (Fig. 18) Five ounce sheet ingots are generally large enough. Any larger and they are too thick to roll down with a standard rolling mill.

The crucible inside an electromelt is carbon, consequently, all alloys can be added at once. Pour as close to the mold as possible to reduce the chance of spillage.

Conclusion on Alloying Process

Alloying 22KT Gold for GranulationFig. 19
Removing wire ingot from mold
If the formula and instructions have been followed, ou will have good ingots ready to use. A good pour as no visible pour lines.

(Fig. 19) There is no oxidation as a result of the layer of soot placed on the mold prior to pouring.

Alloying 22KT Gold for GranulationFig. 20
Wire ingot finished. Spruce has been removed.
With the sprue cut off, the 22kt wire ingot is now ready to forge, roll and draw to desired size. (Fig. 20)

 

Alloying 22KT Gold for GranulationFig. 21
Sheet ingot is finished.
The sheet ingot should be shiny and ready to forge. (Fig 21)

 

Forging Ingots

Alloying 22KT Gold for GranulationFig 22
Forging the ingot
Ingots are somewhat like a sponge and should be compressed before rolling or drawing down. Stress lines and blisters will form on your sheet if the ingot is not forged down properly.

Forge the ingot down to one half the original diameter in order to break down the crystalline structure of the metal before reducing through the rolling mill. (Fig. 22 & Fig. 23)

Alloying 22KT Gold for GranulationFig. 23
Forging the wire ingot
The cast ingot must be forged and annealed repeatedly until is the desired diameter in order to break up its crystalline structure.

After it has been forged down to ½ the original diameter, it is ready to roll or draw down.

Drawing Wire

Alloying 22KT Gold for GranulationFig. 24
Tapering "draw-dog"
Taper a "draw dog" on the end of the wire small enough to fit through the holes on the drawplate.

This can be done by placing two sanding discs face to face on a screw top mandrel (Fig. 24). The drawtongs must have something to grab onto.

Alloying 22KT Gold for GranulationFig. 25
Using a drawplate
Using a drawplate held in a vice, wire may be drawn down to desired size. (Fig. 25)

 

Using The Rolling Mill

Alloying 22KT Gold for GranulationFig. 26
Using a rolling mill
Make sure the ingot and the rolling mill are clean and free of any debris. Any irregularities on the mill rollers will be transferred to the sheet. Start by opening the mill the thickness of the ingot. Pass through once to insure all surfaces are level. Reduce the metal a little at a time with each pass, closing the rollers only one number at a time. Trying to attempt making larger thickness changes will result in stress on the mill and blisters or lines in your metal caused by strain and irregular rolling.

The metal may be reduced by ½ its thickness between each annealing. Once the metal is 2mm or less, anneal every few passes through the rolling mill. (Fig. 26) NEVER rotate the ingot 90 degrees and roll without annealing first. It will cause warping and bulging of your sheet.

By Ronda Coryell – © 2005
All rights reserved internationally. Copyright © Ronda Coryell. Users have permission to download the information and share it as long as no money is made-no commercial use of this information is allowed without permission in writing from Ronda Coryell.